20CrNi3AlMnMo(SM2)鋼的化學(xué)成分�
見表1�
�1 20CrNi3AlMnMo(SM2)鋼化�(xué)成分(質(zhì)量分?jǐn)?shù)�%�
C |
Si |
Mn |
Cr |
Mo |
Ni |
Al |
P |
S |
0.17~0.23 |
≤0.40 |
0.80~1.20 |
0.80~1.20 |
0.20~0.50 |
3.00~3.50 |
1.00~1.50 |
≤0.030 |
0.08~0.15 |
20CrNi3AlMnMo(SM2)鋼的臨界�(diǎn)�
Ac1≈710℃,Ac3≈795�,Ms≈405��
20CrNi3AlMnMo(SM2)鋼的熱加工:
鍛造工藝規(guī)范見�2�
�2 20CrNi3AlMnMo(SM2)鋼鍛造工藝規(guī)�
�(xiàng)� |
加熱溫度/� |
始鍛溫度/� |
終鍛溫度/� |
冷卻方式 |
鋼錠 |
1140~1180 |
1080 |
850 |
緩冷 |
鋼坯 |
1100~1150 |
1040 |
850 |
緩冷 |
20CrNi3AlMnMo(SM2)鋼的�(yù)備熱處理
��20CrNi3AlMnMo(SM2)鋼鍛后不必退��
�、軟化處理工藝:870~930�,油冷,680~700℃高溫回�2h,油�,熱處理后硬�≤30HRC�
20CrNi3AlMnMo(SM2)鋼的固溶處理�
固溶溫度�870~930�,最佳工藝溫度為900℃,油冷,硬度為42~45HRC?;鼗饻囟�?80~700�,油�,硬度為28HRC。固溶回火后硬度較低,便于機(jī)械加��
20CrNi3AlMnMo(SM2)鋼的�(shí)效處理:
�(shí)效溫度為500~520℃,�(shí)效時(shí)間為6~10h,硬度為40HRC�
20CrNi3AlMnMo(SM2)鋼的力學(xué)性能�
力學(xué)性能見表3�
�3 20CrNi3AlMnMo(SM2)鋼力�(xué)性能
熱處理工� |
σb |
σs |
δ5 |
ψ |
αk(J/cm2) |
硬度 |
900℃油��700℃回火油��500~520℃時(shí)�6h |
1176 |
980 |
15 |
45 |
54 |
40 |
900℃油��520℃時(shí)�6~10h |
1147~1196 |
1058~1107 |
11~11.5 |
49~50 |
49~57 |
39~40.5 |